Sheet Metal Galvanic Corrosion & Dissimilar Metals Guide钣金接触腐蚀与异种金属配对指南

A North Sea wind-turbine OEM sent us a warranty claim last year. An outdoor stainless enclosure had been built with a 316L body, a 304 stainless door, and zinc-plated carbon-steel hinges. The hinge pin was 304 stainless. The cabinet had been in service nine months when one of the hinges failed in coastal atmosphere — the hinge pin had corroded into a white powder and snapped under wind load. The zinc plating had been sacrificed to protect the carbon steel, but in doing so it had set up a galvanic cell against the 316L body, which accelerated corrosion at the hinge-body interface. The cabinet had to be pulled, the hinges replaced, and the entire hinge strategy reworked. The redesign used nylon bushings on every hinge pin and insulated washers at every bolt. That fix was free; the field service was not. Below is the DFM playbook that would have prevented it.

This guide covers galvanic corrosion & dissimilar metals for sheet metal enclosures: the galvanic series as it applies to the metals that actually go into sheet metal enclosures, a 6 × 6 pairing matrix for the 30 most common combinations, five suppression methods, environment severity ranking, three real OEM failures, and a seven-item DFM checklist before release.

Why Galvanic Corrosion Matters for Sheet Metal Enclosures

A sheet metal enclosure is rarely built from one metal. The body might be 316L stainless, the door 304 stainless, the hinges zinc-plated carbon steel, the hinge pins 304 stainless, the fasteners A2-70 stainless, and the gland plates aluminum. Every joint between two different metals is a potential galvanic cell — and the cell will deliver current the moment an electrolyte (water, salt fog, humidity) is present. The metal with the lower electrode potential (the "anode") corrodes; the metal with the higher potential (the "cathode") is protected. The rate of corrosion depends on the potential difference between the two metals, the surface area ratio (small anode + large cathode is the worst case), and the aggressiveness of the environment.

Galvanic corrosion is the most under-designed failure mode in the sheet metal enclosure industry. Most engineering drawings specify the body material and the fastener material separately and never check whether the two are compatible. The corrosion shows up in service, usually in the first six to eighteen months, and is attributed to "bad coating" or "bad material" — when the actual root cause was an unfilled compatibility check at the drawing stage. For the broader stainless vs carbon steel comparison, see our stainless vs carbon steel guide, and for the outdoor environment context, our outdoor IP enclosure guide.

The Galvanic Series (Practical Subset for Sheet Metal)

The full galvanic series runs from the most active metals (magnesium, zinc) at the anodic end to the most noble (gold, platinum) at the cathodic end. The sheet metal enclosure designer rarely deals with anything outside a 6-metal subset: magnesium alloys (rare, structural), zinc and zinc-plated steel, aluminum and aluminum alloys, carbon / mild steel, lead, tin, stainless steel, copper / brass, and titanium. Below is the practical galvanic series for these metals in seawater (the most aggressive common environment).

Position (anodic end → cathodic end)Metal / alloyApprox potential vs SHE (V)Common sheet metal form
1 (most anodic)Magnesium alloys-1.55 to -1.75Specialty structural castings (rare)
2Zinc (and zinc-plated steel, galvanized steel)-0.76Galvanized steel sheet, zinc-plated fasteners
3Aluminum alloys (5052, 5083, 6061)-0.75 to -0.95Lightweight enclosures, heat sinks
4Carbon / mild steel (uncoated)-0.55 to -0.70Powder-coated enclosures, brackets
5Lead, tin, tin-plated steel-0.40 to -0.55Solder, tin-plated fasteners
6Stainless steel (304, 316, 316L — passive)-0.05 to -0.15Standard enclosure body / door
7 (most cathodic)Copper, brass, bronze+0.05 to +0.20Brass gland bodies, copper busbars

Three engineering rules for reading the table: (1) the further apart two metals are in the series, the larger the galvanic potential difference, and the worse the corrosion at the anode. Zinc paired with copper (~ 0.8 V difference) is far worse than aluminum paired with stainless (~ 0.6 V difference). (2) The anode corrodes; the cathode does not. So when zinc is paired with stainless, the zinc corrodes — and that is by design if the zinc is a sacrificial plating. The corrosion becomes a problem when the zinc is structural, not sacrificial. (3) A small anode area paired with a large cathode area is the worst geometry — the anode's corrosion current density (amps per square meter) becomes very high. A small stainless fastener on a large carbon steel panel will eat through the fastener before the panel shows visible corrosion. For the broader material selection framework, see our material selection guide.

Pairing Matrix — 30+ Combinations

The table below covers the 30 most common sheet metal enclosure combinations. Each cell shows the corrosion risk and the standard suppression method (if any).

Body / large partFastener / small partRiskStandard suppression
Stainless steelZinc-plated steelHigh (anode zinc)Insulation bushing or replace with stainless fastener
Stainless steelGalvanized steelHigh (anode zinc)Insulation bushing or replace with stainless
Stainless steelAluminumMedium-high (anode Al)Nylon washer, dielectric grease
Stainless steelCarbon steelMedium (anode CS)Insulation washer or replace with stainless
Stainless steelTin-plated steelMedium (anode tin)Insulation washer
Stainless steelStainless steel (same grade)NoneDirect contact OK
Stainless steelStainless steel (different grade)LowDirect contact usually OK; check passivation
Stainless steelBrass / copperMedium-high (anode SS)Insulation washer; SS is the anode here
AluminumZinc-plated steelMedium (anode Zn)Insulation washer; both are sacrificial
AluminumGalvanized steelMediumInsulation washer
AluminumAluminumNoneDirect contact OK; check alloy compatibility
AluminumCarbon steelMedium (anode CS)Insulation washer
AluminumStainless steelHigh (anode Al)Dielectric grease + nylon washer
AluminumBrass / copperHigh (anode Al)Avoid; replace or isolate completely
Carbon steelZinc-plated steelLow (zinc is sacrificial)Direct contact usually OK; the zinc protects the CS
Carbon steelGalvanized steelLowDirect contact OK
Carbon steelAluminumMedium (anode CS or Al depending on environment)Insulation washer or replace
Carbon steelStainless steelHigh (anode CS, small SS fastener)Insulation washer or replace with CS fastener
Carbon steelBrass / copperVery high (anode CS)Avoid; replace with CS fastener
Galvanized steelStainless steelMedium (anode zinc, small SS fastener)Insulation washer; or design so zinc is sacrificial
Galvanized steelAluminumLowDirect contact OK; both are sacrificial
Galvanized steelBrass / copperHigh (anode zinc)Insulation washer; zinc is sacrificial
Tin-plated steelAluminumMediumInsulation washer
Tin-plated steelStainless steelMedium (anode tin)Insulation washer
Tin-plated steelCopper / brassHigh (anode tin)Insulation washer

The matrix is not exhaustive — it covers the 30 combinations that show up on real OEM drawings. For the hinge and latch pairings (where dissimilar metal is the rule rather than the exception), see our hinge & latch selection guide. For the corrosion-coating side that is often used to suppress galvanic corrosion in the first place, see our corrosion coating guide.

5 Suppression Methods (Insulation / Coating / Anode / Spacing / Drainage)

Five engineering methods cover almost every galvanic suppression problem on a sheet metal enclosure. They are listed in order of preference — insulation is the most reliable, drainage the least.

  1. Insulation (electrical isolation). Insert a non-conductive material between the two metals. Nylon washers, nylon bushings, fiberglass gaskets, PTFE (Teflon) sleeves. For fasteners, a nylon washer under the head and a nylon bushing in the hole isolates the two metals. This is the most reliable method and the cheapest to retrofit.
  2. Coating (barrier layer). Paint, powder coat, anodize, or plate one or both of the metals so the electrolyte never reaches the metal surface. Coatings are only as good as their integrity — a scratch in the coating re-creates the cell. For the coating spec, see our corrosion coating guide.
  3. Sacrificial anode. Deliberately place a more active metal (typically zinc) in the joint so that the zinc corrodes instead of the structural metal. Used widely on marine and offshore enclosures. The anode must be replaced periodically — typically every 2–5 years depending on the environment and the anode mass.
  4. Spacing. Keep the two metals physically apart. In a cabinet, this means routing cables, brackets, and supports so they do not bridge dissimilar metals. Not always practical, but free where geometry permits.
  5. Drainage. Design the enclosure so water does not pool at metal-to-metal joints. Sloped surfaces, drain holes, drip edges, and avoiding upward-facing horizontal flanges all reduce the time-of-wetness at the joint. Drainage is the least reliable method on its own but is a useful supplement to any of the first four.

The base is where the severity ranking is least forgiving: anchor, washer, shim and base frame meet in the wettest, least ventilated spot on the cabinet. See dissimilar metals where the anchors meet the base frame.

Environment Severity Ranking

The aggressiveness of the corrosion depends on the environment. The same dissimilar-metal pair that lasts twenty years indoors fails in nine months on a North Sea turbine. The standard severity ranking (ISO 12944 / ISO 9223) is:

Corrosivity categoryTypical environmentSheet metal implication
C1 (very low)Heated indoor spaces, dry atmosphereDirect contact of dissimilar metals acceptable; standard paint OK
C2 (low)Unheated indoor, temperate outdoor (rural)Direct contact OK; galvanized steel acceptable
C3 (medium)Urban / industrial outdoor, coastal with low salinityInsulation on dissimilar-metal joints recommended
C4 (high)Industrial / coastal with moderate salinityInsulation mandatory; powder coat or anodize on aluminum
C5-I (very high, industrial)Heavy industrial, high humidityInsulation + coating + drainage design; consider 316L
C5-M (very high, marine)Coastal / offshore with continuous salt exposure316L body mandatory; insulation mandatory; consider sacrificial anode
CX (extreme)Offshore splash zone, subsea, chemical immersionSpecialty alloys (titanium, super duplex) or non-metallic composite

Two engineering rules apply across all categories: (1) the time-of-wetness is the dominant variable — an enclosure that dries quickly between wet cycles corrodes far less than one that stays wet. Drainage design matters more than coating choice at C3–C5. (2) The galvanic risk is environment-amplified. The same joint that is acceptable at C2 may be unacceptable at C4. For the outdoor IP enclosure context, see our outdoor IP enclosure guide.

3 Real OEM Failures

These three cases are drawn from SanJun's 12-year warranty log, with the customer names anonymized. Each one was traced to a galvanic incompatibility that was not checked at the design stage.

Case 1: North Sea wind turbine hinge failure. 316L body, 304 door, zinc-plated carbon steel hinges, 304 stainless hinge pins. Nine months in C5-M atmosphere; the zinc plating sacrificed itself, accelerated corrosion at the hinge-body interface, and one hinge pin snapped under wind load. Fix: nylon bushings on every hinge pin, insulation washers under every bolt, and a redesign of the hinge to a single 316L part. Field service cost: ~ 8× the original hinge cost.

Case 2: Chemical plant junction box bracket failure. Powder-coated carbon steel junction box body, aluminum bracket for cable gland plate, zinc-plated steel fasteners. Eighteen months in C4-I industrial atmosphere. The aluminum bracket corroded through at the fastener holes (small anode, large cathode, aluminum is the anode). Fix: replace aluminum bracket with stainless bracket, dielectric grease at every fastener interface. Field service cost: ~ 12× the original bracket cost. See our hazardous location guide for the broader chemical plant context.

Case 3: Coastal telecom cabinet door latch failure. Aluminum cabinet body, stainless steel hinge, zinc-plated carbon steel latch body. The zinc latch body was sacrificial in design, but the latch was also small (small anode) and the stainless hinge was large (large cathode). Twelve months in C4-M coastal atmosphere; the latch body had corroded into a powder. Fix: replace zinc latch body with stainless, add nylon washers at the latch mounting points. Field service cost: ~ 6× the original latch cost. For the hinge side of the same problem, see our hinge & latch guide.

DFM — 7 Pre-Release Checks

These seven DFM checks are what we run before releasing a sheet metal drawing that includes dissimilar metals. The first three account for most of the failures we have seen.

  1. List every metal in the assembly. Body, door, hinges, hinge pins, latches, fasteners, gland plates, brackets, ground bars, nameplates, even the rivet material. Each is a potential cell partner with the others.
  2. Mark each metal's position in the galvanic series. Use the table in Section 2. The series position predicts the cell risk.
  3. For every dissimilar-metal joint, identify the anode and the cathode. The anode corrodes. Confirm that the anode is either sacrificial by design (a coating or a planned-replacement anode) or is acceptable to lose (a non-structural bracket).
  4. For every structural anode, specify a suppression method. Insulation washer, dielectric grease, nylon bushing, coating, or anode replacement — and call it out on the drawing with a part number.
  5. For every joint that is not suppressed, document the expected service life. A joint that loses 0.05 mm/year of anode thickness in C3 atmosphere is acceptable for a 5-year design life; it is not acceptable for a 20-year design life. Be honest about it.
  6. Specify the environment corrosivity category on the drawing. C2 / C3 / C4 / C5-I / C5-M. The drawing review and the part approval both depend on this number. For the broader DFM framework, see our DFM design guide.
  7. Specify the fastener material and isolation kit together. "M5 stainless fastener" is not a complete callout. "M5 A2-70 stainless fastener with nylon washer P/N xxx and dielectric grease P/N yyy at every joint to the body" is a complete callout. For the fastener spec side, see our fastener selection guide.

Fasteners deserve a line in that checklist: a pressed insert holds a permanent clamped contact face against the sheet, so the material pairing and isolation rules for pressed inserts should be checked before release.

The SanJun Dissimilar-Metals Workflow

For OEM customers with dissimilar-metal enclosures (especially outdoor / marine / industrial), we run a four-step workflow:

  1. Metal-pair audit. We list every metal in the assembly, mark each one in the galvanic series, and identify every joint that crosses the series.
  2. Suppression spec. For every joint, we specify the suppression method (insulation washer, dielectric grease, coating, anode), with part numbers.
  3. Environment corrosivity review. We confirm the target corrosivity category (C2 / C3 / C4 / C5-I / C5-M) and verify that the suppression spec is rated for that category.
  4. FAI checklist. Every joint is checked at first article inspection — washer present, grease applied, fastener torque recorded. For the prototype-to-volume handoff on dissimilar-metal programs, see our prototype-to-production guide.

The output of the workflow is a one-page Galvanic Compatibility Pack — metal-pair list, suppression spec, environment category, FAI checklist — that goes with every shipment and lets the customer's receiving inspector verify the lot without re-engineering the joint.

Method 2 above assumes the barrier film bonds. It only does so if the conversion stage treated every metal in the assembly, and when one workload carries a steel body, an aluminium subplate and zinc-coated brackets through a single line, a chemistry tuned for one underperforms on the others. That constraint on suppressing the cell is explained in a conversion chemistry that tolerates the whole substrate mix.

Conclusion

A sheet metal enclosure is a stack of dissimilar metals. The stack will corrode in service unless every dissimilar-metal joint is either matched to the galvanic series or explicitly suppressed. The 7 DFM checks above cover the rework we have seen; the matrix above covers the 30 most common combinations; the environment table above covers the severity. If you are at the RFQ stage, send us your environment category (C2 to C5-M), your assembly metal list, and your target service life. We will return a one-page Galvanic Compatibility Pack within 24 hours.

Galvanic compatibility is one input to a wider corrosion decision; the coating systems, the testing and the coastal material choices around it are in the environmental protection cluster.

去年,一位北海风机的 OEM 把一份保修单送过来。一个户外不锈钢外壳,箱体 316L、门板 304、铰链镀锌碳钢、铰链销 304。在沿海大气里用了 9 个月,一个铰链失效了——铰链销锈成白粉,在风载下折了。镀锌层被牺牲去保护碳钢,但这样做时它与 316L 箱体建立了接触腐蚀电池,加速了铰链-箱体界面的腐蚀。柜子得整个拉回来换,所有铰链策略重做。重做时给每个铰链销加了尼龙套、每个螺栓加了绝缘垫。这次修免费;现场服务费不免费。下面这份 DFM 操作手册能避开它。

这篇指南覆盖 galvanic corrosion & dissimilar metals(接触腐蚀与异种金属配对):与钣金外壳实际用到的金属相对应的电偶序、6 × 6 配对矩阵覆盖 30 种最常见组合、五种抑制方法、环境严酷度分级、3 个真实 OEM 失效案例、释放前 7 项 DFM 清单。

为什么接触腐蚀对钣金外壳至关重要

钣金外壳很少只用一种金属。箱体可能是 316L、门板 304、铰链镀锌碳钢、铰链销 304、紧固件 A2-70 不锈钢、密封板铝。两种不同金属之间的每个接缝都是一个潜在的电偶电池——电解质(水、盐雾、潮湿)一出现,电池就开始供电。电极电位低的金属("阳极")腐蚀;电位高的金属("阴极")被保护。腐蚀速率取决于两种金属之间的电位差、面积比(小阳极 + 大阴极是最坏情况)、以及环境的严酷度。

接触腐蚀是钣金外壳行业最被低估的失效模式。多数工程图分别指定箱体材料和紧固件材料,从不检查两者是否相容。腐蚀在使用中出现——通常在头 6 到 18 个月——归因于"涂层差"或"材料差"——但真正的根本原因是图纸阶段没有做相容性检查。碳钢 vs 不锈钢决策那一侧的背景见我们的 不锈钢 vs 碳钢指南,户外环境那一侧见 户外 IP 外壳指南。

电偶序(钣金实用子集)

完整电偶序从最活泼金属(镁、锌)到最贵金属(金、铂)。钣金外壳设计师很少涉及 6 种金属子集以外的:镁合金(少见,结构件)、锌和镀锌钢、铝和铝合金、碳/低碳钢、铅、锡、不锈钢、铜/黄铜、钛。下面是这些金属在海水(最严酷的常见环境)中的实用电偶序。

位置(阳极端 → 阴极端)金属 / 合金相对 SHE 近似电位 (V)常见钣金形式
1(最阳极)镁合金-1.55 到 -1.75专用结构铸件(少见)
2锌(含镀锌钢、镀锌钢板)-0.76镀锌钢板、镀锌紧固件
3铝合金(5052、5083、6061)-0.75 到 -0.95轻量化外壳、散热片
4碳 / 低碳钢(无涂层)-0.55 到 -0.70粉末喷涂外壳、支架
5铅、锡、镀锡钢-0.40 到 -0.55焊料、镀锡紧固件
6不锈钢(304、316、316L — 钝态)-0.05 到 -0.15标准外壳体 / 门
7(最阴极)铜、黄铜、青铜+0.05 到 +0.20黄铜接头体、铜母排

读表的三条工程规则:(1) 两种金属在序中的距离越远,电偶电位差越大,阳极腐蚀越严重。锌配铜(~ 0.8 V 差)远差于铝配不锈钢(~ 0.6 V 差)。(2) 阳极腐蚀、阴极不腐蚀。所以锌配不锈钢时锌腐蚀——如果锌是牺牲镀层,这正是设计意图。问题是当锌是结构件而不是牺牲层时,腐蚀就成了问题。(3) 小阳极面积配大阴极面积是最坏几何——阳极腐蚀电流密度(A/m²)会很高。大碳钢板上的一颗小不锈钢紧固件,会在板子还没可见腐蚀前把紧固件腐蚀穿。材料选型决策的大框架见我们的 材料选型指南。

配对矩阵 — 30+ 组合

下表覆盖 30 种最常见的钣金外壳组合。每个单元格显示腐蚀风险与标准抑制方法(如果有)。

箱体 / 大件紧固件 / 小件风险标准抑制
不锈钢镀锌钢高(阳极锌)绝缘套或换成不锈钢紧固件
不锈钢镀锌钢高(阳极锌)绝缘套或换成不锈钢
不锈钢铝中-高(阳极铝)尼龙垫、绝缘脂
不锈钢碳钢中(阳极 CS)绝缘垫或换成不锈钢
不锈钢镀锡钢中(阳极锡)绝缘垫
不锈钢不锈钢(同牌号)无直接接触可以
不锈钢不锈钢(不同牌号)低直接接触通常可以;检查钝化
不锈钢黄铜 / 铜中-高(阳极 SS)绝缘垫;这里是 SS 作阳极
铝镀锌钢中(阳极锌)绝缘垫;两者都是牺牲阳极
铝镀锌钢中绝缘垫
铝铝无直接接触可以;检查合金相容
铝碳钢中(阳极 CS)绝缘垫
铝不锈钢高(阳极铝)绝缘脂 + 尼龙垫
铝黄铜 / 铜高(阳极铝)避免;替换或完全隔离
碳钢镀锌钢低(锌是牺牲阳极)直接接触通常可以;锌保护 CS
碳钢镀锌钢低直接接触可以
碳钢铝中(环境决定 CS 或铝是阳极)绝缘垫或替换
碳钢不锈钢高(阳极 CS,小 SS 紧固件)绝缘垫或换成 CS 紧固件
碳钢黄铜 / 铜极高(阳极 CS)避免;换成 CS 紧固件
镀锌钢不锈钢中(阳极锌,小 SS 紧固件)绝缘垫;或设计让锌是牺牲阳极
镀锌钢铝低直接接触可以;两者都是牺牲阳极
镀锌钢黄铜 / 铜高(阳极锌)绝缘垫;锌是牺牲阳极
镀锡钢铝中绝缘垫
镀锡钢不锈钢中(阳极锡)绝缘垫
镀锡钢铜 / 黄铜高(阳极锡)绝缘垫

这张矩阵不穷举——它覆盖真实 OEM 图纸上出现的 30 种组合。铰链与锁扣那一侧(异种金属配对是常态而非例外)的细节见我们的 铰链与锁扣选型指南。常用于抑制接触腐蚀本身的涂层那一侧见 腐蚀涂层指南。

5 种抑制方法(绝缘 / 涂层 / 阳极 / 间距 / 排水)

五种工程方法覆盖几乎所有钣金外壳上的接触腐蚀抑制问题。按优先级排——绝缘最可靠,排水最弱。

  1. 绝缘(电隔离)。在两种金属之间插入非导电材料。尼龙垫、尼龙套、玻璃纤维垫、PTFE(特氟龙)套管。对紧固件,在头下加尼龙垫、孔内加尼龙套,把两种金属隔开。这是最可靠的方法,也是改造时最便宜的。
  2. 涂层(屏障层)。在一种或两种金属上刷漆、粉末喷涂、阳极氧化或电镀,使电解质接触不到金属表面。涂层的有效性只与完整性相当——涂层上一道划痕就重建了电池。涂层规格见我们的 腐蚀涂层指南。
  3. 牺牲阳极。故意在接缝处放置更活泼的金属(典型是锌),让锌代替结构金属腐蚀。在海洋与近岸外壳上广泛使用。阳极必须定期更换——典型 2–5 年一次,视环境与阳极质量。
  4. 间距。把两种金属物理隔开。在柜子里,这意味着走线、支架、支撑件不要跨越异种金属。在几何允许时不一定实用,但成本为零。
  5. 排水。把外壳设计成水不会在金属-金属接缝处积聚。斜面、排水孔、滴边、避免向上水平翻边,都减少接缝处的润湿时间。排水单独可靠性最差,但作为前四种的补充很有用。

底座是这套严酷度分级里最不容情的位置:锚栓、垫圈、垫片与底框在最湿、通风最差的一处相遇。见锚栓与底框接触处的异种金属。

环境严酷度分级

腐蚀的严酷度取决于环境。同一个异种金属接缝在户内用 20 年,在北海风机上 9 个月就失效。标准严酷度分级(ISO 12944 / ISO 9223):

腐蚀等级典型环境钣金含义
C1(极低)加热室内空间、干燥大气异种金属直接接触可以;普通油漆可以
C2(低)不加热室内、温带户外(乡村)直接接触可以;镀锌钢可以
C3(中)城市 / 工业户外、低盐度海岸异种金属接缝推荐绝缘
C4(高)工业 / 中等盐度海岸必须绝缘;铝用粉末喷涂或阳极氧化
C5-I(很高,工业)重工业、高湿度绝缘 + 涂层 + 排水设计;考虑 316L
C5-M(很高,海洋)海岸 / 近岸持续盐暴露316L 箱体必须;绝缘必须;考虑牺牲阳极
CX(极端)近岸飞溅区、海底、化学浸没特种合金(钛、特级双相钢)或非金属复合材料

跨等级通用的两条工程规则:(1) 润湿时间是主导变量——干燥快的柜子比始终潮湿的柜子腐蚀少得多。在 C3–C5,排水设计比涂层选择更重要。(2) 接触腐蚀风险随环境放大。同一个接缝在 C2 可接受,在 C4 可能不可接受。户外 IP 外壳的背景见我们的 户外 IP 外壳指南。

3 个真实 OEM 失效案例

这三个案例来自三骏 12 年的保修日志,客户名匿名。每个都追溯到图纸阶段没做接触相容性检查。

案例 1:北海风机铰链失效。316L 箱体、304 门、镀锌碳钢铰链、304 不锈钢铰链销。在 C5-M 大气里 9 个月;镀锌层被牺牲掉,加速铰链-箱体界面腐蚀;一个铰链销在风载下折了。修法:每个铰链销加尼龙套,每个螺栓加绝缘垫,铰链重设计成单一 316L 件。现场服务费:约原铰链成本 8 倍。

案例 2:化工厂接线箱支架失效。粉末喷涂碳钢接线箱体、铝密封板支架、镀锌钢紧固件。在 C4-I 工业大气里 18 个月。铝支架在紧固件孔位腐蚀穿(小阳极、大阴极,铝是阳极)。修法:铝支架换成不锈钢支架,每个紧固件界面加绝缘脂。现场服务费:约原支架成本 12 倍。化工厂更广的背景见我们的 危险场所指南。

案例 3:沿海通讯柜门锁失效。铝柜体、不锈钢铰链、镀锌碳钢门锁体。镀锌门锁体原本设计为牺牲阳极,但门锁体也小(小阳极),不锈钢铰链大(大阴极)。在 C4-M 沿海大气里 12 个月;门锁体腐蚀成粉。修法:镀锌门锁体换成不锈钢,门锁安装点加尼龙垫。现场服务费:约原门锁成本 6 倍。同问题的铰链那一侧见我们的 铰链与锁扣指南。

DFM — 释放前 7 项检查

这 7 项 DFM 检查是我们释放含异种金属的钣金图纸前跑的内容。前 3 项占了我们见过的失效的大半。

  1. 列出装配中的每一种金属。箱体、门、铰链、铰链销、门锁、紧固件、密封板、支架、接地排、铭牌、连铆钉材料。每个都与其他金属组成潜在电池。
  2. 标出每种金属在电偶序中的位置。用第 2 节的表。序中位置预测电池风险。
  3. 对每个异种金属接缝,识别阳极和阴极。阳极腐蚀。确认阳极要么设计为牺牲阳极(涂层或计划更换的阳极),要么可以接受损耗(非结构支架)。
  4. 对每个结构阳极,指定抑制方法。绝缘垫、绝缘脂、尼龙套、涂层、或阳极更换——并在图纸上用料号标注。
  5. 对每个未抑制的接缝,文档化预期使用寿命。C3 大气中年损 0.05 mm 阳极厚度的接缝,5 年设计寿命可接受;20 年设计寿命不可接受。要诚实。
  6. 在图纸上指定环境腐蚀等级。C2 / C3 / C4 / C5-I / C5-M。图评审与零件批准都依赖这个数。大 DFM 框架见我们的 DFM 设计指南。
  7. 紧固件材料与隔离套件一起指定。"M5 不锈钢紧固件"不是完整标注。"M5 A2-70 不锈钢紧固件配 P/N xxx 尼龙垫、P/N yyy 绝缘脂用在每个与箱体的接缝上"才是完整标注。紧固件规格那一侧见 紧固件选型指南。

这份检查表应该给紧固件留一行:压铆件会在板材上留下一个永久压紧的接触面,因此发图前应核对压铆件的材料配对与隔离规则。

三骏的异种金属工作流

对有异种金属外壳(尤其是户外 / 海洋 / 工业)的 OEM 客户,我们跑四步工作流:

  1. 金属配对审计。我们列出装配中的每一种金属,在电偶序中标出每一种,识别每个跨序的接缝。
  2. 抑制规格。对每个接缝,我们指定抑制方法(绝缘垫、绝缘脂、涂层、阳极),附料号。
  3. 环境腐蚀等级评审。我们确认目标腐蚀等级(C2 / C3 / C4 / C5-I / C5-M),验证抑制规格按那个等级合格。
  4. FAI 清单。每个接缝在首件检验时核对——垫片在位、脂涂好、紧固件扭矩记录。异种金属项目从原型到量产的衔接细节见 prototype-to-production 指南。

工作流交付物是一页纸的接触腐蚀相容包——金属配对清单、抑制规格、环境等级、FAI 清单——随每批发货走,让客户收货检验员不用重新设计接缝就能验批次。

上述第 2 种方法默认屏蔽涂层本身能附着。但只有当前处理工序真正处理到总成中的每一种金属时,附着才成立——当一个工件在同一条生产线上同时包含钢制外壳本体、铝制安装板和镀锌支架时,为其中一种金属调好的工艺在其他金属上就会打折。这道限制见能同时覆盖整套基材组合的转化处理工艺。

结语

钣金外壳是一摞异种金属。这摞金属在使用中必然腐蚀,除非每个异种金属接缝要么与电偶序匹配,要么明确抑制。上面 7 项 DFM 检查覆盖我们见过的回工,上面矩阵覆盖 30 种最常见组合,上面环境表覆盖严酷度。如果你在 RFQ 阶段,把环境等级(C2 到 C5-M)、装配金属清单、目标使用寿命发给我们。24 小时内我们回一页纸的接触腐蚀相容包。

电偶相容性只是防腐决策的一项输入;围绕它的涂层体系、试验方法与沿海材料选择见环境防护专题。

Need a Galvanic-Compatibility-Reviewed Sheet Metal Enclosure?需要一份做过接触相容性评审的钣金外壳?

Send us your environment category (C2 to C5-M), your assembly metal list and your target service life. We will return a one-page Galvanic Compatibility Pack within 24 hours.把你的环境等级(C2 到 C5-M)、装配金属清单、目标使用寿命发给我们。24 小时内我们回一页纸的接触腐蚀相容包。